核心摘要:
【高铝砖】
项目 item
单位unit
指标 index
LZ-75
LZ-65
LZ-55
LZ-48
【高铝砖】 |
|
项目 item |
单位 unit |
指标 index |
LZ-75 |
LZ-65 |
LZ-55 |
LZ-48 |
AI2O3≥ |
% |
75 |
65 |
55 |
48 |
耐火度≥ refractoriness |
oC |
1790 |
1790 |
1770 |
1750 |
0.2MPa荷重软化开始温度≥ softening temp under 0.2MPaload |
oC |
1520 |
1500 |
1470 |
1420 |
重烧线变化 linear change of-heating |
1500oC,2h |
% |
+0.1 -0.4 |
|
1450oC,2h |
|
+0.1 -0.4 |
显气孔率≤ porosity |
% |
23 |
22 |
常温耐压温度≥ pressure resistance at normal temp |
Mpa |
53.9 |
49.0 |
44.1 |
39.2 | |